Cycloaliphatic amine epoxy hardener YLH-3002 is a modified cycloaliphatic amine at AHEW 182 g/eq, 5000-12000 cps at 25 °C, and 96 phr on a 190 g/eq resin. Almost half the mixed mass ends up as hardener, and that load sets both the working window and the seven field defects documented in this report.

Transparent pale yellow cycloaliphatic amine hardener YLH-3002 pouring as a thick ribbon into a glass beaker

Figure 1. YLH-3002 as supplied: a transparent liquid thick enough to pour as a rope, at a Gardner colour ceiling of 1.

1. Introduction

Ambient-cure epoxy fails at the mixing bench more often than at the reactor. A hardener that pours at 15 °C and leaves 30 min of working time earns its price.

YLH-3002 sits at the heavy end of the family: 5000-12000 cps and 182 g/eq, far from the 92-100 g/eq flooring grades, and that distance changes metering, air release and the pattern of defects.

Seven defects follow, each with the arithmetic or mechanism behind it, plus where the grade does not fit.

2. Materials and Methods: Cycloaliphatic Amine Epoxy Hardener YLH-3002

2.1 Product Identification and Published Specification

The page publishes no CAS, no formula, no pack size and no shelf life, so identity rests on the batch documents.

Table 1. Identity and commercial data for YLH-3002.

Item

Information

Grade

YLH-3002

Chemical type

Modified cycloaliphatic amine hardener

CAS No.

Not published

Appearance

Transparent viscous liquid

Table 2. Published specification of YLH-3002 at 25 °C.

Property

Value

Colour, Gardner

Max. 1

Viscosity at 25 °C

5000-12000 cps

AHEW

182 g/eq

Amine value

290 mg KOH/g

Density at 25 °C

1.04 g/cm³

Added weight

96 PHR

Table 3. Cure response and mechanical data on a liquid bisphenol A resin of EEW 190.

Test

Result

Gel time, 100 g mix at 25 °C

30 min

Thin film set, 15 g at 3 mm, 25 °C

1.5 h

Shore D 70, 15 g at 3 mm, 25 °C

6 h

Bending failure load

227 N

Bending strength

84.1 MPa

Tensile failure load

2352 N

Tensile strength

54.1 MPa

Table 3 holds only for that resin; a 170 g/eq grade changes phr and cured strength.

2.2 Test Methods and Data Sources

Colour is read according to ASTM D1544, amine value by ISO 9702 titration, water content according to ASTM E203; the page does not say which were run.

Derived values (phr, equivalents per kg, volume ratio) reproduce on a calculator. Mechanical figures carry no standard deviation, so 84.1 MPa is nominal at n = 1.

The amine numbers do not close: 56,100 ÷ 290 = 193.4 g/eq, 6% above the published 182. The phr line settles it: 100 × 182 ÷ 190 = 95.8 matches the published 96, and 193.4 would ask 101.8.

3. Results and Discussion: Hardener Load and Network Density

3.1 What 96 phr Does to the Cured Network

At EEW 190 the 96 phr load puts 95.8 g of hardener against 100 g of bisphenol A resin: hardener is 48.9% of the mix and amine equivalents reach 2.69 per kilogram.

Sibling grades run denser: 3.42 eq/kg for low-viscosity YLH-3023, 3.47 for YLH-6004 polyetheramine hardener, 3.53 for YLH-9101, since 92-100 g/eq equivalents leave less inert mass per crosslink. Hence 21-24% fewer crosslink points, bending at 84.1 MPa against 96.3 MPa, tensile level at 54.1 against 54.0 MPa.

Early hardness breaks the pattern: Shore D 70 in 6 h against 7-15 h, which is kinetics rather than density, since 290 mg KOH/g keeps reactive groups close together.

3.2 Comparison with Alternative Systems

For this cycloaliphatic amine epoxy hardener, specify in one order: viscosity for the process, AHEW for the ratio, equivalents per kg for the network.

Table 4. YLH-3002 against three hardeners from the same catalogue, all on EEW 190.

Property

YLH-3002

YLH-3023

YLH-6004

YLH-9101

AHEW, g/eq

182

100

96

92

Viscosity, 25 °C, cps

5000-12000

250-500

100-300

250-450

Gardner colour, max

1

1

3

2

phr at EEW 190

96

52

50

48

Gel time, 100 g, min

30

30

50

30

Shore D 70, h

6

7

15

8

Bending strength, MPa

84.1

78

96.3

91.7

Amine eq per kg of mix

2.69

3.42

3.47

3.53

A 5000-12000 cps hardener in a plant built for 100-300 cps pumps is a pump problem first. Warm both parts to 30-35 °C and viscosity halves; at 15 °C it starves. If the line cannot be heated, take a 250-500 cps grade.

YLH-3023 and fast-cure YLH-9101 share a 30 min gel yet differ by 13.7 MPa in bending.

4. Formulation and Dosage Calculation

The ratio follows one line: phr = 100 × AHEW ÷ EEW, so 100 × 182 ÷ 190 = 95.8 phr.

Table 5. Hardener demand across the EEW range handled by YLH-3002.

Resin EEW, g/eq

phr by weight

Hardener share

Per 100 kg resin

170

107.1

51.7%

107.1 kg

182

100.0

50.0%

100.0 kg

190

95.8

48.9%

95.8 kg

200

91.0

47.6%

91.0 kg

250

72.8

42.1%

72.8 kg

Hardener is 42-52% of the mixed mass here, so hardener price drives compound cost more than resin price. Moving from EEW 190 to a 170 g/eq bisphenol F grade lifts phr to 107.1, an 11.8% step a fixed 1:1 kit cannot absorb.

By volume the pair sits closer: 95.8 g of hardener at 1.04 g/cm³ fills 92.1 cm³ against 86.2 cm³ of resin, a ratio of 1.07:1.

If a 1:1 volume kit was built for a thinner hardener, it under-doses: one volume to one delivers 1.04 ÷ 1.16 × 100 = 89.7 phr, 6.4% short of 95.8.

5. Processing Notes and Operating Window

Induction earns its minutes. Stand the mix 10-15 min so air can rise while viscosity still allows it; when the shop is cold, allow 20 min.

Weigh both components: a 2% error moves phr two points and leaves the surface tacky for a day while the bulk reads hard.

Temperature sets the clock. The 30 min gel and 1.5 h film set were measured at 25 °C; at 15 °C working life doubles and Shore D 70 takes three times as long. Cap the batch mass: a 25 kg pail gels sooner.

Table 6. Seven field defects, their mechanisms and the corrective action for each.

Symptom

Mechanism

Corrective action

Cost

Greasy, soapy film

Amine plus CO2 and water forms carbamate

Induct 10-15 min, apply 15-25 °C, RH under 75%

Second coat peels

Tacky surface at 24 h

Under-weighed hardener; a 1:1 kit gives 89.7 phr

Meter 96:100 by weight or 1.07:1 by volume

Failed hardness check

Pinholes in a cast

5000-12000 cps holds air; gel closes first

Degas at 5 mbar for 5 min

Voids weaken the section

Bending at 84 MPa, not 96

2.69 eq/kg against 3.5 for thin grades

Specify YLH-6004 where stiffness leads

Overbuilt joints

Gel in a 25 kg pail

The 100 g gel time does not scale

Batches 5-10 kg, or chill to 18 °C

Lost batch

Soft part after 12 °C night

Reactivity falls below 15 °C

20-25 °C for 6 h, or post-cure 60 °C for 2 h

Rework, early release

Bond line lifts on damp steel

Water blocks wetting; blush layer forms

3 °C dew point margin, abrade, solvent-wipe

Adhesive failure

Worker in protective overalls and respirator pouring viscous epoxy hardener into a pail of resin on a workshop floor

Figure 2. Adding hardener at 96 phr: the pour is slow, the induction is not optional, and batch mass is the first thing to cap.

6. Applications

The page lists epoxy adhesives and transparent A/B glue, both leaning on Gardner 1 colour and 54.1 MPa tensile strength.

Table 7. Where YLH-3002 fits and what each process constrains.

Process

Why YLH-3002 fits

Constraint

Transparent two-part adhesive

Gardner 1 keeps a 2-3 mm bond line invisible

30 min gel caps open time

Metal and ABS bonding

54.1 MPa tensile, 227 N bending load

Degrease and abrade; remove blush

Small-part repair

Shore D 70 in 6 h returns the part in one shift

Sections above 10 mm run hot when poured in one shot

Transparent bonding is the natural fit: a 2-3 mm bond line stays invisible and Shore D 70 arrives in 6 h. Deep casting is not, because 5000-12000 cps holds air and 30 min gel leaves no window for degassing.

Clear two-part epoxy adhesive dispensed from a syringe onto a degreased steel bracket beside an ABS part

Figure 3. Clear A/B adhesive on a steel and ABS joint: colour and tensile strength carry the application, viscosity and open time limit it.

7. Limitations and Material Verification

7.1 Known Limitations and Where the Grade Does Not Fit

- No CAS number or formula on the page. Tie identity to the batch COA, not a bare grade name.

- AHEW 182 and amine value 290 mg KOH/g differ by 6%. Pick one basis and record it.

- Chemical resistance is claimed, not quantified; at 2.69 eq/kg check with an immersion test.

- No Tg, HDT or elongation is published, so 84.1 MPa sits off any stiffness curve.

- Not for thin castings, pumps capped at 500 cps, or work below 15 °C.

- Colour drifts in an open drum as Gardner 1 material takes up CO2 and moisture.

7.2 Incoming Inspection, Packaging, Storage and Safety

Verify three numbers on receipt: amine value by ISO 9702 titration, colour according to ASTM D1544, viscosity at 25 °C against the 5000-12000 cps window. Add an ASTM E203 water check if the drum was open or stored cold.

Pack size and shelf life are not published; settle both on the quotation. Storage: ventilated area, clear of flame, cap closed after use.

Safety data belongs in the MSDS; cycloaliphatic amines are corrosive and skin-sensitising by class. RoHS and REACH statements are not published for YLH-3002, so ask per shipment. Where a TDS, MSDS or COA differs from this report, the batch document governs.

8. Frequently Asked Questions

What is the mix ratio of YLH-3002 with a 190 g/eq epoxy resin?

96 phr by weight, or 96 g per 100 g of resin, from 100 × 182 ÷ 190 = 95.8. By volume the pair runs 1.07:1, since the hardener is lighter at 1.04 g/cm³.

Why does YLH-3002 need 96 phr when other cycloaliphatic hardeners need about 50 phr?

AHEW sets it: YLH-3023 at 100 g/eq and YLH-9101 at 92 g/eq carry twice the active hydrogen per gram, so the resin needs half the mass. Networks differ too: 2.69 eq/kg against 3.42-3.53.

Can YLH-3002 be used below 15 °C?

Not without a heated room. The 1.5 h film set and 6 h Shore D 70 were measured at 25 °C, and amine cure slows sharply below that. Hold 20-25 °C for 6 h.

Does YLH-3002 cause amine blush?

It can, on damp days: free amine reacts with CO2 and water into a carbamate that feels soapy and blocks intercoat adhesion. Induction, 15-25 °C and RH under 75% cut most of the risk.

Is YLH-3002 suitable for clear castings and optical parts?

For colour yes, for thickness no. Gardner max 1 keeps a 2-3 mm section clear, but 5000-12000 cps holds air and 30 min gel leaves no time to degas. Bond with it, cast with YLH-3023 at 250-500 cps.

How long does YLH-3002 keep in the drum?

The page publishes no shelf life. Ask for the batch date on the COA, keep the drum closed, and re-run the amine value titration before using older material.

9. Conclusions

YLH-3002 is a 182 g/eq modified cycloaliphatic amine asking 96 phr on a 190 g/eq resin, and delivers 84.1 MPa bending, 54.1 MPa tensile and Shore D 70 in 6 h. Its 5000-12000 cps body and 48.9% share explain most defects seen with it, but the ratio stays a starting point until the COA confirms AHEW.

Three checks cover the common failures: meter 96:100 by weight, hold the shop at 20-25 °C, avoid thick sections. Where stiffness or air release leads, a 92-100 g/eq grade such as YLH-6004 or YLH-6005 modified polyetheramine beats a workaround.

10. References

1. Yolatech product page for YLH-3002: https://www.yolatech.com/curing-agnet-ylh-3002 (accessed 2026-11-17).

2. Yolatech Technical Data Sheet (TDS) for YLH-3002 (available on request).

3. Yolatech Material Safety Data Sheet (MSDS) and Certificate of Analysis (COA) for YLH-3002.

4. ASTM D1544, Gardner color of transparent liquids.

5. ISO 9702, amine group nitrogen content of amine epoxide hardeners.

6. ASTM E203, water content by Karl Fischer titration.

7. Yolatech product page for YLH-3023: https://www.yolatech.com/curing-agnet-ylh-3023 (accessed 2026-11-17).

اترك رسالة

اترك رسالة
إذا كنت مهتما بمنتجاتنا وتريد معرفة المزيد من التفاصيل ، فالرجاء ترك رسالة هنا ، وسوف نقوم بالرد عليك في أقرب وقت ممكن.
إرسال

وطن

منتجات

واتس اب

اتصل بنا